Costing Factors Of Yarn Dyeing Mills

Costing is an important factor. This task is done by the accounts department. They have to calculate the costing of specific products. Generally, the methods of costing are nearly same for all textile departments. But costing depends on the factory types or business types. Sometimes it could be composite mills or sometimes single unit. Anyhow, I have given a short list of costing factor which is applicable for a single yarn dyeing mill.



In a yarn dyeing mill, the raw materials are grey yarn and the finished products are dyed yarn. The business could be run by two ways.


  1. To sale dyed yarn to the buyer. In this case, raw yarn is bought by the mill authority and they dye the grey yarn and sale the finished dyed yarn.

  2. To dye the grey yarn which is supplied by the buyer. In this case, the mill authority fixed a specific dyeing rate for specific yarn. Most of the case, this method is run.


Factors of Costing of a Product: The following factors are considered for costing of any dyed product.

  1. Total dyes and chemical cost

  2. Total utility cost

  3. Salary

  4. Lunch

  5. Entertainment cost

  6. Government cash incentive

  7. Yarn cost

  8. Cost of dyeing

  9. Labor cost (direct & indirect)

  10. Factory cost

  11. Sales and caring cost

  12. Others cost


Above costing factors are the most common. The costing methods could be varying depending on the men’s method. But the basic will be same for all.

So, if you want to calculate the costing, consider the above factors.

Dyed Yarn Drying Process | Drying Mechanism of Stray-field FASTRAN Textile Dryer

Dryer is essential to remove remaining water from the package. About 60-80% water removes by dryer. After passing Hydro section package move into drying section. Following is most used yarn dryer use in yarn dyeing industry.


  1. Stray-field FASTRAN Machine

  2. GALVANIN (Hot Air Dryer)




Drying Mechanism of Stray-field FASTRAN Textile Dryer: There are lots of dyed yarn dryer for drying the dyed yarn which passed hydro-extractor. I have written about the drying mechanism of Stray-field FASTRAN Textile Dryer.

Direct method of heating are those where the heat is generated within the material itself with ratio frequency and microwave method being typical examples. This method of heating is also referred to as dielectric heating.

Most non-metallic substances undergo a uniform rise in temperature when subjected to a high frequency electric magnetic field. Each time the direction of the applied RF field reverse, so the polarization of the individual molecules within the substance changes. The constant molecular movement causes friction which in turn leads to a rise in temperature. As may be expected the higher the frequency of the electromagnetic field the faster the molecules process, thus creating more friction and consequently more heat is produced.

The frequency of the RF fields generated by devices for dielectric heating is centered on 13.50 MHZ and 27.12 MHZ.


Here, I like give a simple idea about the Stray-field FASTRAN Textile Dryer.

Brand Name                : Stray-field

Country Origin             : UK

Supply Voltage            : 380-420

Supply Frequency        : 50 HZ

Supply Phases             : 3

Supply KVA                 : 230

Supply Power Factor    : 0.9

Maximum Weight         : 3800 Kg

RF Power Output         : 100 kW

Operating Frequency    : 27 MHZ

Points Need to Consider During Drying: Following points are need to consider during yarn drying. They are:

  1. Machine Speed: Machine speed varies according to the shade of the yarn. Conveyor runs in high speed for dark shade and comparatively at low speed for light shade.

  2. Feeding System: Plastic package feed in vertical form, but spring package feed in horizontal form because fire can be form by feeding in vertical form.

  3. Yarn Type: Same type yarn should run at same settings. Otherwise it can damage the yarn quality. Cotton, Polyester, Acrylic, P/C or CVC yarn should feed separately.

  4. Moisture: Machine settings should be according to the amount of moisture remain in the package.


Evaluation of Efficiency of Stray-field Dryer: It needs to know the efficiency of a dyed yarn dryer. For this reason, I have presented a sample calculation of dyed yarn dryer efficiency.

Weight of double yarn package before dyeing               =  1.2 Kg

Weight of double yarn package with water before Dryer = 2.034 Kg

Weight of water in double yarn package before Dryer = (2.034 – 1.2) Kg =  0.834 Kg

Weight of package after Dryer          =          1.2 Kg

Water remain in package after Dryer   =          (1.2 – 1.2) Kg =  0 Kg

Water remove by Dryer                     =          (0.834 – 0) Kg = 0.834kg

Efficiency

=   {(Weight of water before Dryer - Water remain after Dryer) / Weight of water before Dryer}   X 100%

=   {(0.834 – 0) / 0.834} X 100%

=    1 X 100%

=    100 %

Efficiency of Dryer = 100 %

So, yarn dryer is essential for dry the dyed yarn. After drying, dyed yarns transferred for re-winding or random section.

Process Flow Chart Of Polyester Dyeing | Disperse Dyes Dyeing Process

Polyester is the most used synthetic fiber of the world. Polyester fiber is dyed with disperse dyes. If we want, we can dye the fiber during yarn preparation. Also we can dye the yarn after yarn preparation and in fabric form. The fastness properties of polyester dyed yarn are excellent. Day by day the use of synthetic fiber increases rapidly.

Process Flow Chart Of Polyester | Disperse Dye Dyeing ProcessDyeing sequence of polyester is given below:

Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add washing agent and run at 800 C for 20 min


↓


Dyeing period


↓


Add leveling agent and acid, run at 600 C for 10 min


↓


PH check


↓


Color mixing at 700 C for 40 min


↓


Color dosing at 600 C for 20 min


↓


Polyester dyeing at 1350 C at 20 gradient for 50 min


↓


Sample check


↓


Ok


↓


Temperature cool down at 780 C and drain


↓


Hot wash for 10 min


↓


Rinse for 15 min for light shade and 25 min for dark shade


↓


Add hydrose, soda ash, run at 800 C for 20 min


↓


Drain


↓


Rinse for 10 min


↓


Neutralization by acetic acid at 500 C 20 min


↓


Finishing


So, that’s all about the polyester dyeing as well as synthetic yarn dyeing. You can try it in your practical life and give me a feedback about the result of dyeing process of polyester.

Dyeing Flow Chart of Polyester Cotton | Two Part Dyeing Process

Dyeing sequence of polyester cotton is the combination of polyester and cotton dyeing process. For this reason this dyeing process is called double part dyeing process. In this dyeing process; polyester part is dyed first than cotton part is dyed.

Dyeing flow chart of polyester cotton is given below:

 Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add wetting agent, antifoaming agent, sequestering agent and run at 600 C for 10 min


↓


Water solution drain


↓


Add wetting agent, sequestering agent, caustic soda and hydrogen peroxide and run at 1100 C for single yarn and 1150 C for double yarn for 20 min


↓


Drain


↓


Add peroxide killer and run at 900 C for 10 min


↓


Peroxide check in the package


↓


Drain


↓


Add acetic acid for neutralization and run for 20 min at 500 C


↓


Drain


↓


Take sample and check absorbency


↓


Ok


↓


Dyeing period (Polyester part)


↓


Add leveling agent and acid, run at 600 C for 10 min


↓


PH check


↓


Color mixing at 700 C for 40 min


↓


Color dosing at 600 C for 20 min


↓


↓


Sample check


↓


Ok


↓


Temperature cool down at 780 C and drain


↓


Hot wash for 10 min


↓


Rinse for 15 min for light shade and 25 min for dark shade


↓


Add hydrose, soda ash, run at 800 C for 20 min


↓


Drain


↓


Neutralization by acetic acid at 500 C 20 min


↓


Take sample


↓


Carbonizing by acid for 10-20 min


↓


Neutralization by acetic acid at 500 C for 20 min


↓


Drain


↓


Dyeing of polyester part complete


↓


Dyeing period (Cotton part)


↓


Add wetting agent, antifoaming agent, sequestering agent and run at 600 C for 10 min


↓


Color dosing at 600 C for 20 min


↓


Color migration at 600 C for 30 min


↓


Salt dosing at 600 C for 20 min


↓


Run the machine for 20 min at 600 C with color and salt


↓


Soda dosing at 600 C for 40 min


↓


Cotton dyeing at 600 C for 50 min


↓


Check sample


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add acetic acid for neutralization and run for 10 min at 500 C


↓


Drain


↓


Add washing chemical and run at 900 C for 20 min


↓


Wash sample check


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add fixing chemical and half acetic acid, run at 500 C for 20 min


↓


Add softening agent and rest half acid, run at 600 C for 20 min


↓


Check finished sample


↓


Ok


↓


Drain


It is note that; dyeing sequence of CVC is as same as P/C dyeing. If we want to dye cvc then we can run the process as same the above process sequence.

Dyeing Sequence Of 100% Cotton With Turquoise Color | Dark Shade

Shade of the textile materials depends on the dyes percentage which is used for dyeing. Chemical which is used for dyeing also vary depending on the dyes used. Generally dark shade means the dyes percentage above 2%. Medium shade dyeing and dark shade dyeing process is nearly same.

Flow chart of cotton dyeing with turquoise color is given below:

 Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add wetting agent, antifoaming agent, sequestering agent and run at 600 C for 10 min


↓


Water solution drain


↓


Add wetting agent, sequestering agent, caustic soda and hydrogen peroxide and run at 1100 C for single yarn and 1150 C for double yarn for 20 min


↓


Drain


↓


Add peroxide killer and run at 900 C for 10 min


↓


Peroxide check in the package


↓


Drain


↓


Add acetic acid for neutralization and run for 20 min at 500 C


↓


Drain


↓


Absorbency test of sample


↓


Ok


↓


Dyeing period


↓


Add salt, wetting agent, antifoaming agent, sequestering agent and run at 600 C for 10 min


↓


PH check


↓


Color dosing at 600 C for 30 min


↓


Color migration at 800 - 900  C for 30 min


↓


Migration package check


↓


Ok


↓


Run the machine for 20 min at 800 - 900 C with color and salt


↓


Soda dosing at 600 C for 40 min


↓


Cotton dyeing at 800 - 900 C for 50 min


↓


Check sample


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add acetic acid for neutralization and run for 10 min at 500 C


↓


Drain


↓


Add washing chemical and run at 950 C for 20 min


↓


Add washing chemical and run at 900 C for 20 min


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add fixing chemical and half acetic acid, run at 500 C for 20 min


↓


Add softening agent and rest half acid, run at 600 C for 20 min


↓


Check finished sample


↓


Ok


↓


Drain


So, dye your textile materials with turquoise color and get the colorful yarns or fabrics.

Dyeing Flow Chart of Cotton With Turquoise Color | Light Shade

Turquoise color dyeing is critical than the normal color dyeing. This type of dyes is used for produce specific color. A flow chart of turquise color dyeing for light shade is given below:

 Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add wetting agent, anti foaming agent, sequestering agent and run at 600 C for 10 min


↓


Water solution drain


↓


Add wetting agent, sequestering agent, caustic soda and hydrogen peroxide and run at 1100 C for single yarn and 1150 C for double yarn for 20 min


↓


Drain


↓


Add peroxide killer and run at 900 C for 10 min


↓


Peroxide check in the package


↓


Drain


↓


Add acetic acid for neutralization and run for 20 min at 500 C


↓


Drain


↓


Absorbency test of sample


↓


Ok


↓


Dyeing period


↓


Add wetting agent, antifoaming agent, sequestering agent and run at 600 C for 10 min


↓


Color dosing at 600 C for 20 min


↓


Color migration at 800 - 900 C for 30 min


↓


Salt dosing at 600 C for 20 min


↓


Run the machine for 20 min at 800 - 900 C with color and salt


↓


Soda dosing at 600 C for 40 min


↓


Cotton dyeing at 800 - 900 C for 50 min


↓


Check sample


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add acetic acid for neutralization and run for 10 min at 500 C


↓


Drain


↓


Add washing chemical and run at 900 C for 20 min


↓


Wash sample check


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add fixing chemical and half acetic acid, run at 500 C for 20 min


↓


Add softening agent and rest half acid, run at 600 C for 20 min


↓


Check finished sample


↓


Ok


↓


Drain


 It’s too much practical; if you want you can try in cotton dyeing for light shade. Don’t forget to inform me about the results.

Dyeing Flow Chart for Acrylic Yarn | Synthetic Fiber Dyeing

In dyeing floor different types of yarn or fabrics are dyed. All of the process is not same. But the basic dyeing process is same for yarn or fabrics.

Acrylic Yarn dyeing process is given below:

 Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add washing agent and run at 800 C for 20 min


↓


Dyeing period


↓


Add leveling agent and acid, run at 600 C for 10 min


↓


PH check


↓


Color mixing at 700 C for 40 min


↓


Color dosing at 600 C for 20 min


↓


Acrylic dyeing at 850 C at 20 gradient for 20 min


↓


Acrylic dyeing at 980 C at 10 gradient for 50 min


↓


Sample check


↓


Ok


↓


Temperatures cool down at 780 C and drain


↓


Rinse for 15 min for light shade and 25 min for dark shade


↓


Add acetic acid, soda ash, run at 800 C for 20 min


↓


Drain


↓


Rinse for 20 min


↓


Finishing


During acrylic dyeing; temperature plays an important role. Temperatures are up and down according to the requirement.

 

Dyeing Flow Chart For Acrylic Cotton | Yarn Dyeing Process

Dyeing is the most critical task for a textile engineer. Acrylic cotton dyeing is the double part dyeing process. Here dyeing is done one part to another. It needs to match cotton part and acrylic part then dyeing will be completed.

Flow chart of acrylic cotton dyeing is as follow:

Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add wetting agent, anti foaming agent, sequestering agent and run at 600 C for 10 min


↓


Water solution drain


↓


Add wetting agent, sequestering agent, soda ash and hydrogen peroxide and run at 1100 C for single yarn and 1150 C for double yarn for 20 min


↓


Drain


↓


Add peroxide killer and run at 900 C for 10 min


↓


Peroxide check in the package


↓


Drain


↓


Add acetic acid for neutralization and run for 20 min at 500 C


↓


Drain


↓


Take sample and check absorbency


↓


Ok


↓


Dyeing period (Acrylic part)


↓


Add leveling agent and acid, run at 600 C for 10 min


↓


PH check


↓


Color mixing at 700 C for 40 min


↓


Color dosing at 600 C for 20 min


↓


Acrylic dyeing at 850 C at 20 gradient for 20 min


↓


Acrylic dyeing at 980 C at 10 gradient for 50 min


↓


Sample check


↓


Ok


↓


Temperature cools down at 780 C and drain


↓


Rinse for 15 min for light shade and 25 min for dark shade


↓


Add acetic acid, soda ash, run at 800 C for 20 min


↓


Drain


↓


Rinse for 20 min


↓


Take sample


↓


Carbonizing by acid for 10-20 min


↓


Neutralization by acetic acid at 500 C for 20 min


↓


Acrylic part dyeing complete


↓


Dyeing period (Cotton part)


↓


Add wetting agent, antifoaming agent, sequestering agent and run at 600 C for 10 min


↓


Color dosing at 600 C for 20 min


↓


Color migration at 600 C for 30 min


↓


Salt dosing at 600 C for 20 min


↓


Run the machine for 20 min at 600 C with color and salt


↓


Soda dosing at 600 C for 40 min


↓


Cotton dyeing at 600 C for 50 min


↓


Check sample


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add acetic acid for neutralization and run for 10 min at 500 C


↓


Drain


↓


Add washing chemical and run at 900 C for 20 min


↓


Wash sample check


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add fixing chemical and half acetic acid, run at 500 C for 20 min


↓


Add softening agent and rest half acid, run at 600 C for 20 min


↓


Check finished sample


↓


Ok


↓


Drain


 

So, this is the process of acrylic cotton dyeing. Try it in practical and let me know the result.

Dyeing Flow Chart Of Grey Melange || Scouring And Bleaching Process

Grey Melange yarn is the special types of yarn. The fabric which is made from the grey melange yarn is also special. Here I have given a dyeing flow chart by which grey melange yarns are dyed. After dyeing grey melange yarns are used for producing woven and knitted fabrics. Dyeing also done for grey melange fabric but basic dyeing sequence is same.



Dyeing flow chart for grey melange is given below:

Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add wetting agent, anti foaming agent, sequestering agent and run at 600 C for 10 min


↓


Water solution drain


↓


Add wetting agent, sequestering agent, caustic soda, hydrogen peroxide, optical brightening agent and run at 900 C for single yarn and 1000 C for double yarn for 40 min


↓


Drain


↓


Add peroxide killer and run at 900 C for 10 min


↓


Peroxide check in the package


↓


Drain


↓


Add acetic acid for neutralization and run for 20 min at 500 C


↓


Drain


↓


Add washing chemical and run at 900 C for 20 min


↓


Wash sample check


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add fixing chemical and half acetic acid, run at 500 C for 20 min


↓


Add softening agent and rest half acid, run at 600 C for 20 min


↓


Check finished sample


↓


Ok


↓


Drain


 

Day by day the use of grey melange increased rapidly. The dyeing sequence which is given above is carried out for yarn dyeing.

 

White Dyeing | Dyeing Flow Chart of Scouring and Bleaching With Optical Brightening Agent (OBA)

Dyeing is carried out for changing the appearance of the grey yarn or fabric. Generally dyeing is done with the help of dyes and chemical. Most of the time raw materials become colorful by the application of dyes. But if we want to get a white fabric we need to pass through the wet processing methods. The methods by which we can get white materials that method are called white dyeing. Generally white dyeing is carried out with the optical brightening agent during scouring and bleaching process.



I have given a flow chart of white dyeing by which we can get a white dyed yarn. The process is as bellow:

Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add wetting agent, anti foaming agent, sequestering agent and run at 600 C for 10 min


↓


Water solution drain


↓


Add wetting agent, sequestering agent, caustic soda, hydrogen peroxide, optical brightening agent and run at 1100 C for single yarn and 1150 C for double yarn for 40 min


↓


Drain


↓


Add peroxide killer and run at 900 C for 10 min


↓
Peroxide check in the package


↓


Drain


↓


Add acetic acid for neutralization and run for 20 min at 500 C


↓


Drain


So, it is the most practical procedure of white dyeing. If you have better idea about this process let me know.

Dyeing Sequence of 100% Cotton for Medium and Dark Shade | Yarn Dyeing Process

In dyeing; process sequence can be vary depending on the shade of the material which is required to produce. I have given a process sequence for the light shade dyeing but basic sequence is almost same. Now I like to give a process flow chart of dyeing for medium and dark shade.

Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add wetting agent, antifoaming agent, sequestering agent and run at 600 C for 10 min


↓


Water solution drain


↓


Add wetting agent, sequestering agent, caustic soda and hydrogen peroxide and run at 1100 C for single yarn and 1150 C for double yarn for 20 min


↓


Drain


↓


Add peroxide killer and run at 900 C for 10 min


↓


Peroxide check in the package


↓


Drain


↓


Add acetic acid for neutralization and run for 20 min at 500 C


↓


Drain


↓


Absorbency test of sample


↓


Ok


↓


Dyeing period


↓


Add salt, wetting agent, antifoaming agent, sequestering agent and run at 600 C for 10 min


↓


PH check


↓


Color dosing at 600 C for 30 min


↓


Color migration at 600 C for 30 min


↓


Migration package check


↓


Ok


↓


Run the machine for 20 min at 600 C with color and salt


↓


Soda dosing at 600 C for 40 min


↓


Cotton dyeing at 600 C for 50 min


↓


Check sample


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add acetic acid for neutralization and run for 10 min at 500 C


↓


Drain


↓


Add washing chemical and run at 950 C for 20 min


↓


Add washing chemical and run at 900 C for 20 min


↓


Wash sample check


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add fixing chemical and half acetic acid, run at 500 C for 20 min


↓


Add softening agent and rest half acid, run at 600 C for 20 min


↓


Check finished sample


↓


Ok


↓


Drain


So, If anyone wants to get the prove, he can apply this technique in yarn dyeing process for producing medium and dark shade on 100% cotton. Please, let me know the results.

Quality Assurance System at Different Stages of Yarn Dyeing | Quality Measuring System

In every production floor there have a quality department which is responsible for ensuring the quality of the product. In yarn dyeing floor there have a quality department. Textile engineer or a quality officer measures the quality of the product by carrying different quality test.



The value of a product is depends on the quality. Different types of qualities are checked for various products. For yarn dyeing floor; the quality of the dyed yarns are measured as the following flow chart:

Dyed yarn from production section with batch card


↓


Yarn dried by passing it hydro extractor and dryer


↓


Take six layer of a package in random section


↓


Determine the levelness of yarn package (Single yarn)


↓


Take knitting of a package as the sequence (outer + middle + inner) for double yarn


↓


Match the layer and knitting with the standard swatch


↓


Ok


↓


Approved from Q.C


↓


Take wash and rubbing fastness report


↓


Ok


↓


Approved from Q.C


↓


Take pass or fail report from data color


↓


Ok


↓


Approved from Q.C


↓


Product is ready for delivery


In dyeing; different types of dyeing faults could be happened. It is the responsibility of a quality officer to find it out and gives the solution to remove that’s faults. After passing the all types of quality test, a product becomes ready for the delivery.

Considering Points For Packing And Delivery Section Of Yarn Dyeing Floor

Packing Section: In Packing section; dyed yarn packages are packed after passing the re winding section. During packing various types of packing materials are used. It is the final steps before delivery. Quality control officer ensure the quality of the dyed yarn before packing.

Points Need to Consider During Pack: A sticker is added to the package which bears important information about that’s package. Following points are considered for making a sticker.


  • Buyer’s name

  • Work order

  • Count

  • Shade name

  • Batch number

  • Quantity


External Material Used during Packing: During packing, various types of packing accessories are used. Following packing accessories are used for dyed yarn pack.

  • Plastic bag

  • Poly bag

  • Plastic rope

  • Sticker

  • Marker


Delivery Section: After completing the packing work yarns are stored for the delivery. It is work of store section. In delivery section, materials are delivered as per schedule of delivery.

Point Needs to Consider in Delivery Section: Following points are considered during delivery.

  • Delivery section maintains the register.

  • Delivery invoice or challan and gate-pass should maintain.

  • Delivery clearance should provide to the delivery section.

  • For single yarn party consider 4% process loss.

  • Delivery section should keep daily and monthly report.


So, that’s all about the packing and delivery section of a yarn dyeing floor.

 

Process Flow Chart For 100% Cotton Yarn Dyeing | Light Shade Cotton Dyeing (Less Than 1%)

In yarn dyeing floor; process for cotton yarn can be vary depending on the individual procedure of a textile engineer or a dyeing master. I have given a process flow chart for 100% cotton dyeing. This sequence is applicable for producing light shade (less than 1%).

Dyeing sequence for 100% cotton for light shade:

Carrier and vessel washed by hydrose and caustic at 1000 C for 20 min


↓


Load the package in the carrier and feed in the vessel


↓


Add wetting agent, anti foaming agent, sequestering agent and run at 600 C for 10 min


↓


Water solution drain


↓


Add wetting agent, sequestering agent, caustic soda and hydrogen peroxide and run at 1100 C for single yarn and 1150 C for double yarn for 20 min


↓


Drain


↓


Add peroxide killer and run at 900 C for 10 min


↓


Peroxide check in the package


↓


Drain


↓


Add acetic acid for neutralization and run for 20 min at 500 C


↓


Drain


↓


Absorbency test of sample


↓


Ok


↓


Dyeing period


↓


Add wetting agent, anti foaming agent, sequestering agent and run at 600 C for 10 min


↓


Color dosing at 600 C for 20 min


↓


Color migration at 600 C for 30 min


↓


Salt dosing at 600 C for 20 min


↓


Run the machine for 20 min at 600 C with color and salt


↓


Soda dosing at 600 C for 40 min


↓


Cotton dyeing at 600 C for 50 min


↓


Check sample


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add acetic acid for neutralization and run for 10 min at 500 C


↓


Drain


↓


Add washing chemical and run at 900 C for 20 min


↓


Wash sample check


↓


Ok


↓


Drain


↓


Rinse for 10 min


↓


Add fixing chemical and half acetic acid, run at 500 C for 20 min


↓


Add softening agent and rest half acid, run at 600 C for 20 min


↓


Check finished sample


↓


Ok


↓


Drain


 

Oh, my friends this is my own observation if you have better one let me know the sequence of cotton dyeing for light shade. I think this will give you a better way to get better dyeing performance.

Re-Winding Section Of Yarn Dyeing Floor | Objectives And Considering Points Of Re-Winding

Re-winding is the last steps of yarn dyeing process. The process which is started by soft winding section, it comes in end by re winding section. After re winding, dyed yarns become ready for packing and delivery to the destination.



In yarn dyeing floor re-winding section is also called random section. In this section dried and dyed yarns are transferred from spring or plastic tube to cone form.

Objectives: The objectives of re-winding are given bellow:


  1. To transfer the dyed yarn from tube or spring to cone package.

  2. To clean the yarn.

  3. To make the yarn in continuous form.

  4. To prepare the cone package for the delivery.


Re-Winding machine: In re-winding section, various types of machines are used. One of the most used re-winding machine is GAO14; GROOVED DRUM WINDER which is manufacture by SUZHOU XINSAFANG MECHNICAL & ELECTRICAL. The origin country of this machine is China. It contains 100 Spindle.

Points Need to Consider During Re-winding: During re-winding process various points are considered which are given bellow:

  1. Trash: Trash is one of the big problems in random section. Different shaded yarns are re-wind in random section, so color trash fly in the section and enter into package of other color or same color, which destroy the quality of the package. Especially it is harmful for the white or off white color, where other color trash can be identify easily.

  2. Wax: Waxes use in random section. Yarn passes through the wax. Wax gives softness and lubricity of the yarn, which facilities better knitting performance.

  3. Tension: Tension is given to double yarn not in single yarn. Because tension makes single yarn package hard.

  4. Wet Package: Wet package should not re-wind because wet package become hard after re-winding. It also makes beets in the cone package.

  5. Cone: Cone should be available.

  6. Blower: Blower should work properly, because cleaning performance depends on blower performance.

  7. Operator: Operator should aware about the cleanliness.


That’s all about re-winding section. One should be aware about the re-winding process and produce fault free product for the buyer.

Working Mechanism Of Hydro-Extractor | Evaluation Of Efficiency Of Hydro-Extractor

In yarn dyeing process; hydro extractor section plays an important role after passing dyeing section. Hydro extractor which is used for package yarn is different from the hydro extractor which is used for fabric.

Hydro-extractor is essential to remove excess water from the package. About 60-70% water removes by hydro-extractor. After passing dyeing section package enter into Hydro-extractor section.



Machine Description: It needs to know about a machine before using it. So before selection of a machine, ones should get the information which is given bellow. I have presented a machine profile with some data which is essential to know.

Brand Name      : DETTINS.P.A

Country Origin   : ITALY

Model              : BERTA 24 T.E

Rotation          : 1500 rpm (Maximum)

No. of Arm       : 04

No. of Spindle   : 64

Power             : 15, 8 kW

Alimentation     : 400 Volts, 50 HZ

Working Mechanism of Hydro-Extractor: Every manufacturer supplies a prospectus in which they supply all information about the machine and its working procedure. I have described the working mechanism of a hydro extractor by my working experience. Dyed yarn package placed on spindle then entered into basket. The basket consists of a central spindle on which the head of the arm is placed. The wall of the basket is perforated. The basket rotates at high rate of speed up to 1500 rpm. The excess water is removed by the centrifugal force. Up to 70% water is removed by this machine. Then yarn package transferred into dryer.

Evaluation of Efficiency of Hydro-Extractor: It needs to evaluate the efficiency of a hydro extractor because it determines the working power of a hydro extractor. For this reason I like to give an evaluation process of efficiency of a hydro extractor.

Let,

Weight of double yarn package before dyeing                 =          1.2 Kg

Weight of double yarn package with water before Hydro   =   3.49 Kg

Weight of water in double yarn package before Hydro       = (3.49 – 1.2) Kg

=  2.29 Kg

 

Weight of package after Hydro         =  2.034 Kg

Water remain in package after Hydro =  (2.034 – 1.2) Kg  =  0.834 Kg

Water remove by Hydro-Extractor     =  (2.29 – 0.834) Kg =  1.456 kg

 

Efficiency  = {(Weight of water before Hydro - Water remain after Hydro) - Weight of water before Hydro} X 100%

= {(2.29 – 0.834) - 2.29} X 100%

= 0.63 X 100%

= 63%

Efficiency of Hydro-Extractor = 63%

After passing hydro-extractor section yarn packages are send to dryer section for removing remaining water.

So, using of a hydro extractor should be perfect. Also we have to care full about the fault which could be occur during this process.

Common Yarn Dyeing Faults | Causes And Way Of Remedies

Dyeing is the combination of reaction among fiber, dyes, chemicals and water. In dyeing process different faults can be occur for various factor. Among all of the dyeing process, package yarn dyeing is different. In package yarn dyeing different types of faults are occurs but following are the most common.


Uneven dyeing: A textile engineer must have knowledge about the shade of color. Small percentage of shade difference can move a material to rejection. So, it needs to be high care full during dyeing. Dyeing is a continuous process and during dyeing ones should be sure about the shade of materials that it matched with the standard swatch. Uneven shade means the variation of shade in different layer of a yarn package. We know that package yarn dyeing is done by the In-0ut mechanism of dye liquor. So shade could be varying in various layer of a package. Followings are the causes and remedies of uneven shade.

Causes:

→ Uneven pretreatment (uneven scouring & bleaching).

→ Improper color dosing.

→ Using dyes of high fixation property.

→ Uneven heat-setting in case of synthetic fibers.

→ Lack of control on dyeing m/c


Remedies:

→ By ensuring even pretreatment.

→ By ensuring even heat-setting in case of synthetic fibers.

→ Proper dosing of dyes and chemicals.

→ Proper controlling of dyeing m/c.

Batch to Batch Shade variation: In dyeing; dyeing is done according to the buyer requirement. An order for a specific shade could be small amount or large amount. In mill, different batch is made as per order or depending on the capacity of the machine. For this reason batch to batch shade variation could be take place. Followings are the causes and remedies way of batch to batch variation.

Causes:

→ Fluctuation of Temperature.

→ Improper dosing time of dyes & chemicals.

→ Batch to batch weight variation of dyes and chemicals.

→ Dyes lot variation.

→ Improper reel speed, pump speed, liquor ratio.

→ Improper pretreatment.

Remedies:

→ Use standard dyes and chemicals.

→ Maintain the same liquor ratio.

→ Follow the standard pretreatment procedure.

→ Maintain the same dyeing cycle.

→ Identical dyeing procedure should be followed for the same depth of the Shade.

→ Make sure that the operators add the right bulk chemicals at the same time and temperature in the process.

→ The pH, hardness and sodium carbonate content of supply water should check daily.

So, friends make sure about the yarn dyeing faults and take steps for remove it.

Peroxide, Absorbency And pH Test During Dyeing | Test Carried Out For Better Dyeing

In dyeing process different test is carried out to determine the better dyeing. We know that per oxide is applied during bleaching and it is harmful for human body. So it needs to remove from the yarn or fabric. Some points are need to consider during dyeing. Absorbency and pH test is essential for dyeing and it checks during dyeing. A short description of some test is given bellow.



Test carried out during dyeing process


  • Peroxide Test: This test is carried out after bleaching process. This test determines the amount of peroxide present in yarn or fabric. It requires to make sure that material is peroxide free because peroxide is harmful for the yarn or fabric. A peroxide test paper is used. Wet yarn package or fabric is used for this. The test stick is hiding in the middle for 15-20 sec. then takes out from the package or fabric and match with the test scale. If color change then it contains peroxide. If color don’t change then there have no peroxide.

  • Absorbency Test: Absorbency test is carried out after bleaching. At first sample is dried and immerse into water. Standard time for absorbency is up to 5 sec. Better absorbency of sample facilities better dyeing operation.

  • PH Test: It needs to control PH of the dyeing bath, because it affects the exhaustion and fixation rate. Some dyeing process is carried out in alkaline medium and some are carried out in acidic medium. Generally natural fibers dyeing are carried out in alkaline medium and synthetic fibers dyeing are carried out in acidic medium. It also depends on dyes characteristics and what’s type of dyes are used for which fiber. In practical way following parameters are maintained for dyeing cotton and polyester and in different stage of dyeing PH level vary.


PH levels for different stages of cotton dyeing

  1. Initial Bath pH                                                   :6.5~7.0

  2. Before Enzyme, bath pH                                     :4.5~4.7

  3. After Enzyme & Aquachoron ,pH                           :5.5~6.0

  4. Before Scouring & Bleaching, pH (With Enzyme)      :5.5~5.8

  5. Before Scouring & Bleaching, pH (Without Enzyme)  :5.5~5.8

  6. Scouring & Bleaching, bath pH                          :10.0~10.5

  7. After Scouring & Bleaching, pH                             :8.5~9.0

  8. Before Leveling Chemicals, pH                              :6.5~7.0

  9. After Leveling Chemicals, pH                                :6.7~7.0

  10. After Adding Dyes, pH                                     :6.2~6.35

  11. After Addition of Salt, pH                                  :7.5~8.0

  12. After Addition of Soda, pH                              :10.5~11.0

  13. Before Hot Wash, Bath pH                                 :6.8~7.2

  14. Hot Wash, bath pH                                          :8.5~8.7


PH levels for different stages of polyester dyeing:

1.   Initial bath pH                                                        :6.5~7.0

2.   Scouring, bath pH                                                :10.0~11.5

3.   After Scouring, bath pH                                           :8.5~9.0

4.   Before Addition of Leveling Chemicals, pH                    :6.0~6.5

5.   After Addition of Leveling Chemicals, pH                      :4.5~4.7

6.   After Addition of Colors, bath pH                                :4.2~4.3

7.   During Reduction Clearing, bath pH                          :10.5~11.5

8.   Before Softener, bath pH                                           :6.3~6.8

9.   After Softener Addition, bath pH                                :5.8~6.2

So, that’s all about the test carried out during dyeing. It also increases the dyeing efficiency and these test should carried out during dyeing.

 

Points Need To Consider During Yarn Dyeing Process | Influencing Factor Of Yarn Dyeing

Yarn dyeing process is different from knit dyeing or woven dyeing. During dyeing, textile engineer should give deep concern on the following points. He should give proper instruction to his supervisor or operator to do all the work as per schedule. If any faults occur during dyeing process then it will impact on the dyeing process. In package yarn dyeing process following points are important to consider.

Batch:


  1. Batching should be done by same lot yarn and same count yarn.

  2. Package level after pressing should be uniform.

  3. Package cap should be tight, it should not loose during operation in the dye bath.


Pressure:

  1. In-Out and Out-In pressure for each machine should maintain. If pressure vary than In-Out and Out-In will not be uniform, which after the levelness of package.

  2. Pressure should maintain during level in and level out process.



PH:

PH is one the most important factor in dyeing process. Following is the PH which should maintain for Cotton:

After salt mixing        : PH 6-6.5

After soda mixing      : PH 11-11.5

After process PH should be neutral.

Checking:

→Checking is important. Checking should be performed in every step of operation.

→Sample checking should be after

● Bleaching (Residue H2O2, Absorbency check)

● Color migration (Level check)

● Dyeing

● Washing

● Finishing

→Water level should check.

→Carrier batch should check after every step by open the lid.

→Time and temperature should check.

Measurement: Operator/Supervisor should be aware during measurement. One should be aware about the measurement because a small mistake can vary the shade of the materials.

● Dyes measurement

● Chemical measurement

● Water measurement

● Time measurement

● Temperature measurement

So, if a respective person aware about the points then he or she will get success in dyeing. Let do the same and see the results.

Functions Of Chemical Auxiliaries Used In Wet Processing | List Of Chemical Auxiliaries

We know that dyes and chemicals are the main factor for producing color in yarn of fabric. Different types of chemicals are used during dyeing. In different stages of dyeing processing, various chemicals are used. Every chemical have their own characteristics and they are used in different stages of wet processing.



List of Chemical auxiliaries used in wet processing unit and their function is given bellow:


  1. Acid: Acid is used to control PH. Acid decrease the pH of the solution. If PH 1-7 then it is called Acidic solution.

  2. Basic: Basic is used for increase the PH of the solution. PH range of basic is 7-14. This also used as scouring agent.

  3. Peroxide Killer: This chemical is used to kill per oxide which is remaining in the material. Peroxide is harmful for the material. A test is carried out to measure the amount of peroxide present in the solution.

  4. Bleaching Agent: Bleaching is carried out before dyeing or printing operation. Better absorption of dyes depends on better bleaching. Absorbency test is carried out to test the bleaching performance. Absorbency time should lie under 5 second. It is used for removing natural color from the grey yarn or fabric.

  5. Salt/Electrolyte: Salt is used as electrolyte. Salt increase the exhaustion rate of the dyeing process. Different types of salt are used for different shade. The amount of salt used depends on the shade % of the material.

  6. Scouring Agent: Scouring agent is used to remove fat, waxes, fragments of cotton etc.

  7. Antifoaming Agent: Foam is formed during bleaching and dyeing process. Anti foaming agent is used to resist foam formation. If foam formed it reduces the dyeing uptake %.

  8. Sequestering Agent: This agent is used to remove hardness of water.

  9. Dispersing Agent: This agent is used for disperse dyes. We know, disperse dye is insoluble in water and dye present in disperse form. By applying this agent dye molecule breaks and become soluble in the solution.

  10. Neutralization Agent: This agent is used to neutral the PH of the solution.

  11. Wash/Soaping Agent: Soaping agent is used for washing. It needs to wash dyed material to remove unfix dye from the material. Dark material needs double wash. But light shade materials needs single wash, sometimes no wash is carried out for light shade. It also increases the reflecting properties.

  12. Softening Agent: This agent is used to increase softness of the material. This agent used as finishing material.

  13. Fixing Agent: This agent is used for fixing of dyestuff and also remove the unfix dye.

  14. Brightening Agent: This agent is used to increase the brightness of the material. This agent increases the reflecting property of the material. Standard reflecting value is 85%. But sometimes it is possible to increase it up to 95%. But it is risk because it needs high kier boiler temperature, which reduces the strength of material.